Processing Parameters (appliable to MiniSTAR®, MiniSTAR®S, and Biostar®)

Thickness(mm)

Temperature()

Heating time(s)

Pressure(bar)

0.40

220

15-20

3.2-3.5

0.63

220

25-30

3.5-4.0

0.76

220

30-35

3.5-4.2

1.00

220

30-40

3.8-4.5

Processing Parameters (appliable to Druformat Scan &Erkodent®Units)

Thickness(mm)

Temperature()

Pressure time(s)

0.76

170-180

30-40

Note: Heating times vary between different machines.

Ø  If the plastic sheet doesn’t form well to the model, add 3-5 seconds on heating time until confirmation is acceptable.

Ø  Please be aware that higher pressure and/or longer heating time may cause the risk of a thinner aligner.

Ø  If the plastic forms folds or abnormal deformation, reduce the heating time until folds do not occur.